Our firm since its inception, normally regards item top quality as company life, constantly make improvements to generation technology, improve product excellent and repeatedly strengthen organization total good quality management, in strict accordance with the national standard ISO 9001:2000 for High Temperature Alloy Seamless Tube/ Pipe, Good quality and competitive prices make our products enjoy a high reputation all over the word. The credibility is the priority, and the service is the vitality. We promise we now have the ability to provide excellent quality and reasonable price products for customers. With us, your safety is guaranteed.
SCM415 is a grade of Japanese steel, which is equivalent to 15CrMo of domestic grades and 15CrMo4 of ISO-693-17-1999. The steel is a low-carbon alloy steel with high thermal strength and oxidation resistance, as well as good comprehensive mechanical properties. Alloy structural steel, used in boilers and steam turbines for superheater tubes, steam tubes and corresponding forgings of high-pressure boilers below 530℃.
SCM415 Chemical Component:
Tensile strength σb (MPa): ≥440(45)
Yield strength σs (MPa): ≥295(30)
Elongation δ5 (%): ≥22
15CrMo Chemical Component:
C: 0.12 ~ 0.18
Mn: 0.40 ~ 0.70
Si: 0.17 ~ 0.37
Cr: 0.80 ~ 1.10
Mo: 0.40 ~ 0.55
Ni: ≤0.30
S: ≤0.035
P: ≤0.035
15CrMo Mechanical Property:
Tensile strength MPa: 440~640
Yield point MPa: 295
Elongation (%): 22
We can find 15CrMo and SCM415 is similiar, is there is no special requirement, the two can substitute for each other
Application
It Is Mainly Used To Make Carbon Structural Steel, Alloy Structural Steel and mechanical structures.
Main Grade
Grade Of Carbon Structural Steel: 10,20,35, 45,Q345,Q460,Q490,Q620,, Etc
Grade Of Alloy Structural Steel: 42CrMo,35CrMo, Etc
Chemical Component
Steel Grade |
Quality level |
Chemical composition |
||||||||||||||
C |
Si |
Mn |
P |
S |
Nb |
V |
Ti |
Cr |
Ni |
Cu |
Nd |
Mo |
B |
Als" |
||
no greater than |
not less than |
|||||||||||||||
Q345 | A |
0.20 |
0.50 |
1.70 |
0.035 | 0.035 |
0.30 |
0.50 |
0.20 |
0.012 |
0.10 |
—— | — | |||
B | 0.035 | 0.035 | ||||||||||||||
C | 0.030 | 0.030 |
0.07 |
0.15 |
0.20 |
0.015 |
||||||||||
D |
0.18 |
0.030 | 0.025 | |||||||||||||
E | 0.025 | 0.020 | ||||||||||||||
Q390 | A |
0.20 |
0.50 |
1.70 |
0.035 | 0.035 |
0.07 |
0.20 |
0.20 |
0.3 |
0.50 |
0.20 |
0.015 |
0.10 |
— | — |
B | 0.035 | 0.035 | ||||||||||||||
C | 0.030 | 0.030 |
0,015 |
|||||||||||||
D | 0.030 | 0.025 | ||||||||||||||
E | 0.025 | 0.020 | ||||||||||||||
Q42O | A |
0.20 |
0.50 |
1.70 |
0.035 | 0.035 |
0.07 |
0.2 |
0.20 |
0.30 |
0.80 |
0.20 |
0.015 |
0.20 |
—— |
—— |
B | 0.035 | 0.035 | ||||||||||||||
C | 0.030 | 0.030 |
0.015 |
|||||||||||||
D | 0.030 | 0.025 | ||||||||||||||
E | 0.025 | 0.020 | ||||||||||||||
Q46O | C |
0.20 |
0.60 |
1.80 |
0.030 | 0.030 |
0.11 |
0.20 |
0.20 |
0.30 |
0.80 |
0.20 |
0.015 |
0.20 |
0.005 |
0.015 |
D | 0.030 | 0.025 | ||||||||||||||
E | 0.025 | 0.020 | ||||||||||||||
Q500 | C |
0J8 |
0.60 |
1.80 |
0.025 | 0.020 |
0.11 |
0.20 |
0.20 |
0.60 |
0.80 |
0.20 |
0.015 |
0.20 |
0.005 |
0.015 |
D | 0.025 | 0.015 | ||||||||||||||
E | 0.020 | 0.010 | ||||||||||||||
Q550 | C |
0.18 |
0.60 |
2.00 |
0.025 | 0,020 | 0.11 |
0.20 |
0.20 |
0.80 |
0.80 |
0.20 |
0.015 |
0.30 |
0.005 |
0.015 |
D | 0.025 | 0,015 | ||||||||||||||
E | 0.020 | 0.010 | ||||||||||||||
Q62O | C |
0.18 |
0.60 |
2.00 |
0.025 | 0.020 |
0.11 |
0.20 |
0.20 |
1.00 |
0.80 |
0.20 |
0.015 |
0.30 |
0.005 |
0.015 |
D | 0.025 | 0.015 | ||||||||||||||
E | 0.020 | 0.010 | ||||||||||||||
a. In addition to Q345A and Q345B grades, the steel should contain at least one of the refined grain elements Al, Nb, V, and Ti. According to the needs, the supplier can add one or more refined grain elements. The maximum value shall be as specified in the table. When combined, Nb + V + Ti is not more than 0.22%b. For Q345, Q390, Q420 and Q46O grades, Mo + Cr is not greater than 0.30%c. When Cr and Ni of each grade are used as residual elements, the content of Cr and Ni should not be greater than 0.30%; when it is necessary to add, the content should meet the requirements in the table or be determined by the supplier and the buyer through consultation.d. If the supplier can ensure that the nitrogen content meets the requirements in the table, the nitrogen content analysis may not be performed. If Al, Nb, V, Ti and other alloy elements with nitrogen fixation are added to the steel, the nitrogen content is not limited. The nitrogen fixation content should be specified in the quality certificate.e. When using full aluminum, the total aluminum content Alt ≥ 0020%. |
Grade |
Carbon equivalent CEV (mass fraction) /% |
|||||
Nominal wall thickness s≤ 16mm |
Nominal wall thickness S2>16 mm〜30 mm |
Nominal wall thickness S>30mm |
||||
Hot rolled or normalized normalized |
Quenching +tempering |
Hot rolled or normalized |
Quenching +tempering |
Hot rolled or normalized |
Quenching +tempering |
|
Q345 |
<0.45 |
— |
<0.47 |
— |
<0.48 |
一 |
Q390 |
<0.46 |
一 |
W0.48 |
— |
<0.49 |
— |
Q420 |
<0.48 |
一 |
<0.50 |
<0.48 |
<0.52 |
<0,48 |
Q460 |
<0.53 |
<0.48 |
W0.55 |
<0.50 |
<0.55 |
W0.50 |
Q500 |
一 |
<0.48 |
一 |
<0.50 |
一 |
W0.50 |
Q550 |
— |
<0.48 |
.一 |
<0.50 |
一 |
<0.50 |
Q62O |
— |
<0.50 |
— |
<0.52 |
— |
W0.52 |
Q690 |
— |
<0.50 |
— |
<0.52 |
— |
W0.52 |
Mechanical Property
Mechanical properties of high-quality carbon steel structural steel and low-alloy high-strength structural steel pipes
Grade | Quality level | Yield Strength | Lower yield strength | Elongation after breaking | Impact test | |||
Nominal wall thickness | temperature | Absorb energy | ||||||
<16 mm | >16 mm〜 | 〉30 mm | ||||||
30 mm | ||||||||
not less than | not less than | |||||||
10 | — | >335 | 205 | 195 | 185 | 24 | — | — |
15 | — | >375 | 225 | 215 | 205 | 22 | — | 一 |
20 | —— | >410 | 245 | 235 | 225 | 20 | — | — |
25 | — | >450 | 275 | 265 | 255 | 18 | — | — |
35 | — | >510 | 305 | 295 | 285 | 17 | 一 | — |
45 | — | 2590 | 335 | 325 | 315 | 14 | — | — |
20Mn | —• | >450 | 275 | 265 | 255 | 20 | — | 一 |
25Mn | — | >490 | 295 | 285 | 275 | 18 | — | — |
Q345 | A | 470—630 | 345 | 325 | 295 | 20 | — | 一 |
B | 4~20 | 34 | ||||||
C | 21 | 0 | ||||||
D | -20 | |||||||
E | -40 | 27 | ||||||
Q39O | A | 490—650 | 390 | 370 | 350 | 18 | ||
B | 20 | 34 | ||||||
C | 19 | 0 | ||||||
D | -20 | |||||||
E | -40 | 27 | ||||||
Q42O | A | 520〜680 | 420 | 400 | 380 | 18 | ||
B | 20 | 34 | ||||||
C | 19 | 0 | ||||||
D | -20 | |||||||
E | -40 | 27 | ||||||
Q46O | C | 550〜720 | 460 | 440 | 420 | 17 | 0 | 34 |
D | -20 | |||||||
E | -40 | 27 | ||||||
Q500 | C | 610〜770 | 500 | 480 | 440 | 17 | 0 | 55 |
D | -20 | 47 | ||||||
E | -40 | 31 | ||||||
Q550 | C | 670〜830 | 550 | 530 | 490 | 16 | 0 | 55 |
D | -20 | 47 | ||||||
E | -40 | 31 | ||||||
Q62O | C | 710〜880 | 620 | 590 | 550 | 15 | 0 | 55 |
D | -20 | 47 | ||||||
E | -40 | 31 | ||||||
Q690 | C | 770〜94。 | 690 | 660 | 620 | 14 | 0 | 55 |
D | -20 | 47 | ||||||
E | -40 | 31 |
Mechanical properties of alloy steel pipes
NO | Grade | Recommended heat treatment regime | Tensile properties | Annealed or high temperature tempered steel pipe Delivery condition Brinell hardness HBW | ||||||
Quenching (normalizing) | Tempering | Yield StrengthMPa | Tensile Strength MPa | Elongation after breaking A% | ||||||
temperature | Coolant | Temperature | Coolant | |||||||
Frirst | Second | not less than | no greater than | |||||||
1 | 40Mn2 | 840 | Water, oil | 540 | Water, oil | 885 | 735 | 12 | 217 | |
2 | 45Mn2 | 840 | Water,oil | 550 | Water, oil | 885 | 735 | 10 | 217 | |
3 | 27SiMn | 920 | Water | 450 | Water, oil | 980 | 835 | 12 | 217 | |
4 | 40MnBc | 850 | oil | 500 | Water, oil | 980 | 785 | 10 | 207 | |
5 | 45MnBc | 840 | oil | 500 | Water, oil | 1 030 | 835 | 9 | 217 | |
6 | 20Mn2Bc'f | 880 | oil | 200 | Water, air | 980 | 785 | 10 | 187 | |
7 | 20CrdJ | 880 | 800 | Water,oil | 200 | Water, air | 835 | 540 | 10 | 179 |
785 | 490 | 10 | 179 | |||||||
8 | 30Cr | 860 | oil | 500 | Water, oil | 885 | 685 | 11 | 187 | |
9 | 35Cr | 860 | oil | 500 | Water, oil | 930 | 735 | 11 | 207 | |
10 | 40Cr | 850 | oil | 520 | Water, oil | 980 | 785 | 9 | 207 | |
11 | 45Cr | 840 | oil | 520 | Water, oil | 1 030 | 835 | 9 | 217 | |
12 | 50Cr | 830 | oil | 520 | Water, oil | 1 080 | 930 | 9 | 229 | |
13 | 38CrSi | 900 | oil | 600 | Water, oil | 980 | 835 | 12 | 255 | |
14 | 20CrModJ | 880 | Water,oil | 500 | Water, oil | 885 | 685 | 11 | 197 | |
845 | 635 | 12 | 197 | |||||||
15 | 35CrMo | 850 | oil | 550 | Water, oil | 980 | 835 | 12 | 229 | |
16 | 42CrMo | 850 | oil | 560 | Water, oil | 1 080 | 930 | 12 | 217 | |
17 | 38CrMoAld | 940 | Water, oil | 640 | Water, oil | 980 | 835 | 12 | 229 | |
930 | 785 | 14 | 229 | |||||||
18 | 50CrVA | 860 | oil | 500 | Water, oil | 1 275 | 1 130 | 10 | 255 | |
19 | 2OCrMn | 850 | oil | 200 | Water、air | 930 | 735 | 10 | 187 | |
20 | 20CrMnSif | 880 | oil | 480 | Water, oil | 785 | 635 | 12 | 207 | |
21 | 3OCrMnSif | 880 | oil | 520 | Water, oil | 1 080 | 885 | 8 | 229 | |
980 | 835 | 10 | 229 | |||||||
22 | 35CrMnSiA£ | 880 | oil | 230 | Water、air | 1 620 | 9 | 229 | ||
23 | 20CrMnTie-f | 880 | 870 | oil | 200 | Water、air | 1 080 | 835 | 10 | 217 |
24 | 30CrMnTie*f | 880 | 850 | oil | 200 | Water、air | 1 470 | 9 | 229 | |
25 | 12CrNi2 | 860 | 780 | Water,oil | 200 | Water、air | 785 | 590 | 12 | 207 |
26 | 12CrNi3 | 860 | 780 | oil | 200 | Water、air | 930 | 685 | 11 | 217 |
27 | 12Cr2Ni4 | 860 | 780 | oil | 200 | Water、air | 1 080 | 835 | 10 | 269 |
28 | 40CrNiMoA | 850 | —— | oil | 600 | Water、air | 980 | 835 | 12 | 269 |
29 | 45CrNiMoVA | 860 | — | oil | 460 | oil | 1 470 | 1 325 | 7 | 269 |
a. Allowable adjustment range of heat treatment temperature listed in the table: quenching ± 15 ℃, low temperature tempering ± 20 ℃, high temperature tempering soil 50 ℃.b. In the tensile test, transverse or longitudinal samples can be taken. In case of disagreement, the longitudinal sample is used as the basis for arbitration.c. Boron-containing steel can be normalized before quenching, and the normalizing temperature should not be higher than its quenching temperature.d. Delivery according to a set of data specified by the demander. When the demander has not specified, delivery can be made according to any of the data.
e. The first quenching of titanium steel with Ming Meng can be replaced by normalizing. f. Isothermal quenching at 280 C ~320 C. g. In the tensile test, if Rel cannot be measured, Rp0.2 can be measured instead of Rel. |
Test Requirement
Chemical composition:
Stretch,Hardness,Shock,Squash,Bending,Ultrasonic testing,Eddy current,detection,Leak detection,Galvanized