Ixabiso elona lihle kwi-China yoLwakhiwo kunye noKwakha iCarbon Steel Pipe GB 8162
Sihlala siwufeza umoya wethu ''wokusungula izinto ezintsha ezisa uphuhliso, umgangatho ophezulu wokuqinisekisa ukuziphilisa, ulawulo olukhuthaza inzuzo, ukutsalwa kwetyala abathengiUmbhobho wentsimbi yeCarbon, Umbhobho wentsimbi, umbhobho wesakhiwo, umbhobho wentsimbi yesakhiwo, Siphuhlise iimarike ezinkulu kumazwe amaninzi, anje ngeYurophu neUnited States, eMpuma Yurophu naseMpuma Asia. Ngeli xesha kukho ukongamela okunamandla kubantu abanesakhono, ulawulo olungqongqo lwemveliso kunye neshishini concept.we sihlala siqhubeka nokuzakhela izinto ezintsha, ukusungula izinto ezintsha zobuchwepheshe, ukulawula ukuqamba izinto ezintsha kunye nokucinga kweshishini. Ukulandela ifashoni yeemarike zehlabathi, iimpahla ezitsha zigcinwa kuphando kunye nokubonelela ukuqinisekisa ukukhuphisana kwethu kwizimbo, umgangatho, ixabiso kunye nenkonzo.
Isishwankathelo
Isicelo
Isetyenziselwa ikakhulu ukwenza iCarbon Structural Steel, i-alloy Structural Steel kunye nezakhiwo zoomatshini.
IBanga eliPhambili
IBanga leCarbon Structural Steel: 10,20,35, 45,Q345,Q460,Q490,Q620, njl.
IBanga leNsimbi yoLwakhiwo lwe-alloy: 42CrMo, 35CrMo, njl.
ICandelo leMichiza
IBanga leNsimbi | Inqanaba lomgangatho | Ukuqulunqwa kweekhemikhali | ||||||||||||||
C | Si | Mn | P | S | Nb | V | Ti | Cr | Ni | Cu | Nd | Mo | B | Als" | ||
akukho mkhulu kune | hayi ngaphantsi kwe | |||||||||||||||
Q345 | A | 0.20 | 0.50 | 1.70 | 0.035 | 0.035 | 0.30 | 0.50 | 0.20 | 0.012 | 0.10 | —- | - | |||
B | 0.035 | 0.035 | ||||||||||||||
C | 0.030 | 0.030 | 0.07 | 0.15 | 0.20 | 0.015 | ||||||||||
D | 0.18 | 0.030 | 0.025 | |||||||||||||
E | 0.025 | 0.020 | ||||||||||||||
Q390 | A | 0.20 | 0.50 | 1.70 | 0.035 | 0.035 | 0.07 | 0.20 | 0.20 | 0.3 | 0.50 | 0.20 | 0.015 | 0.10 | - | - |
B | 0.035 | 0.035 | ||||||||||||||
C | 0.030 | 0.030 | 0,015 | |||||||||||||
D | 0.030 | 0.025 | ||||||||||||||
E | 0.025 | 0.020 | ||||||||||||||
Q42O | A | 0.20 | 0.50 | 1.70 | 0.035 | 0.035 | 0.07 | 0.2 | 0.20 | 0.30 | 0.80 | 0.20 | 0.015 | 0.20 | —- | —- |
B | 0.035 | 0.035 | ||||||||||||||
C | 0.030 | 0.030 | 0.015 | |||||||||||||
D | 0.030 | 0.025 | ||||||||||||||
E | 0.025 | 0.020 | ||||||||||||||
Q46O | C | 0.20 | 0.60 | 1.80 | 0.030 | 0.030 | 0.11 | 0.20 | 0.20 | 0.30 | 0.80 | 0.20 | 0.015 | 0.20 | 0.005 | 0.015 |
D | 0.030 | 0.025 | ||||||||||||||
E | 0.025 | 0.020 | ||||||||||||||
Q500 | C | 0j8 | 0.60 | 1.80 | 0.025 | 0.020 | 0.11 | 0.20 | 0.20 | 0.60 | 0.80 | 0.20 | 0.015 | 0.20 | 0.005 | 0.015 |
D | 0.025 | 0.015 | ||||||||||||||
E | 0.020 | 0.010 | ||||||||||||||
Q550 | C | 0.18 | 0.60 | 2.00 | 0.025 | 0,020 | 0.11 | 0.20 | 0.20 | 0.80 | 0.80 | 0.20 | 0.015 | 0.30 | 0.005 | 0.015 |
D | 0.025 | 0,015 | ||||||||||||||
E | 0.020 | 0.010 | ||||||||||||||
Q62O | C | 0.18 | 0.60 | 2.00 | 0.025 | 0.020 | 0.11 | 0.20 | 0.20 | 1.00 | 0.80 | 0.20 | 0.015 | 0.30 | 0.005 | 0.015 |
D | 0.025 | 0.015 | ||||||||||||||
E | 0.020 | 0.010 | ||||||||||||||
a.Ukongeza kwi-Q345A kunye ne-Q345B amabakala, intsimbi kufuneka iqulethe ubuncinane enye yezinto eziziinkozo ezicocekileyo i-Al, Nb, V, kunye ne-Ti. Ngokweemfuno, umthengisi unokongeza enye okanye ngaphezulu kwezinto eziziinkozo ezicocekileyo. Elona xabiso liphezulu liyakuba njengoko lichaziwe kwitheyibhile. Xa idibene, i-Nb + V + Ti ayikho ngaphezu kwe-0.22%b. Kwi-Q345, Q390, Q420 kunye ne-Q46O amabakala, i-Mo + Cr ayikho ngaphezu kwe-0.30%c. Xa i-Cr kunye ne-Ni yebakala ngalinye zisetyenziswa njengezinto ezishiyekileyo, umxholo we-Cr no-Ni akufanele ube mkhulu kune-0.30%; xa kuyimfuneko ukongeza, umxholo kufuneka uhlangabezane neemfuno kwitheyibhile okanye unqunywe ngumthengisi kunye nomthengi ngokubonisana.d. Ukuba umthengisi unokuqinisekisa ukuba umxholo we-nitrogen uhlangabezana neemfuno kwitheyibhile, uhlalutyo lomxholo we-nitrogen alunakwenziwa. Ukuba i-Al, i-Nb, i-V, i-Ti kunye nezinye izinto ze-alloy kunye nokulungiswa kwe-nitrogen zongezwa kwintsimbi, umxholo we-nitrogen awukhawulelwanga. Umxholo wokulungiswa kwenitrogen kufuneka ucaciswe kwisiqinisekiso somgangatho.e. Xa usebenzisa i-aluminium epheleleyo, umxholo we-aluminium opheleleyo Alt ≥ 0020%. |
IBanga | ICarbon elingana ne-CEV (iqhezu lobunzima) /% | |||||
Ubukhulu bodonga lwegama s≤ 16mm | Ubukhulu bodonga lwegama S2>16 mm〜30 mm | Ubukhulu bodonga lwegama S>30mm | ||||
Ishushu iqengqeleke okanye iqhelekile | Ukucima +ukucaphuka | Ishushu iqengqeleke okanye iqhelekile | Ukucima +ukucaphuka | Ishushu iqengqeleke okanye iqhelekile | Ukucima +ukucaphuka | |
Q345 | <0.45 | - | <0.47 | - | <0.48 | 一 |
Q390 | <0.46 | 一 | W0.48 | - | <0.49 | - |
Q420 | <0.48 | 一 | <0.50 | <0.48 | <0.52 | <0,48 |
Q460 | <0.53 | <0.48 | W0.55 | <0.50 | <0.55 | W0.50 |
Q500 | 一 | <0.48 | 一 | <0.50 | 一 | W0.50 |
Q550 | - | <0.48 | .一 | <0.50 | 一 | <0.50 |
Q62O | - | <0.50 | - | <0.52 | - | W0.52 |
Q690 | - | <0.50 | - | <0.52 | - | W0.52 |
IPropati yoomatshini
Iipropathi zeMechanical ezikumgangatho ophezulu wekhabhoni yentsimbi yolwakhiwo kunye nemibhobho yentsimbi yolwakhiwo olusezantsi-amandla aphezulu
IBanga | Inqanaba lomgangatho | Unikeze Amandla | Amandla esivuno esisezantsi | Ukunyuka emva kokuphuka | Uvavanyo lwempembelelo | |||
Ubukhulu bodonga lwegama | ubushushu | Funxa amandla | ||||||
<16 mm | >16 mm〜 | 〉30 mm | ||||||
30 mm | ||||||||
hayi ngaphantsi kwe | hayi ngaphantsi kwe | |||||||
10 | - | >335 | 205 | 195 | 185 | 24 | - | - |
15 | - | >375 | 225 | 215 | 205 | 22 | - | 一 |
20 | —- | >410 | 245 | 235 | 225 | 20 | - | - |
25 | - | > 450 | 275 | 265 | 255 | 18 | - | - |
35 | - | >510 | 305 | 295 | 285 | 17 | 一 | - |
45 | - | 2590 | 335 | 325 | 315 | 14 | - | - |
20Mn | —• | > 450 | 275 | 265 | 255 | 20 | - | 一 |
25Mn | - | >490 | 295 | 285 | 275 | 18 | - | - |
Q345 | A | 470—630 | 345 | 325 | 295 | 20 | - | 一 |
B | 4~20 | 34 | ||||||
C | 21 | 0 | ||||||
D | -20 | |||||||
E | -40 | 27 | ||||||
Q39O | A | 490—650 | 390 | 370 | 350 | 18 | ||
B | 20 | 34 | ||||||
C | 19 | 0 | ||||||
D | -20 | |||||||
E | -40 | 27 | ||||||
Q42O | A | 520〜680 | 420 | 400 | 380 | 18 | ||
B | 20 | 34 | ||||||
C | 19 | 0 | ||||||
D | -20 | |||||||
E | -40 | 27 | ||||||
Q46O | C | 550〜720 | 460 | 440 | 420 | 17 | 0 | 34 |
D | -20 | |||||||
E | -40 | 27 | ||||||
Q500 | C | 610〜770 | 500 | 480 | 440 | 17 | 0 | 55 |
D | -20 | 47 | ||||||
E | -40 | 31 | ||||||
Q550 | C | 670〜830 | 550 | 530 | 490 | 16 | 0 | 55 |
D | -20 | 47 | ||||||
E | -40 | 31 | ||||||
Q62O | C | 710〜880 | 620 | 590 | 550 | 15 | 0 | 55 |
D | -20 | 47 | ||||||
E | -40 | 31 | ||||||
Q690 | C | 770〜94. | 690 | 660 | 620 | 14 | 0 | 55 |
D | -20 | 47 | ||||||
E | -40 | 31 |
Iimpawu zomatshini wemibhobho yensimbi ye-alloy
NO | IBanga | Ulawulo lonyango olucetyiswayo | Iimpawu zokuqina | Umbhobho wentsimbi ene-anealed okanye ubushushu obuphezulu obupholileyo Imeko yonikezelo Ubulukhuni beBrinell HBW | ||||||
Ukucinywa (okuqhelekileyo) | Ukufudumeza | Yield StrengthMPa | Amandla e-Tensile MPa | Ukwandiswa emva kokwaphulwa kwe-A% | ||||||
ubushushu | Ukupholisa | Ubushushu | Ukupholisa | |||||||
Okokuqala | Isibini | hayi ngaphantsi kwe | akukho mkhulu kune | |||||||
1 | 40Mn2 | 840 | Amanzi, ioli | 540 | Amanzi, ioli | 885 | 735 | 12 | 217 | |
2 | 45Mn2 | 840 | Amanzi, ioli | 550 | Amanzi, ioli | 885 | 735 | 10 | 217 | |
3 | 27SiMn | 920 | Amanzi | 450 | Amanzi, ioli | 980 | 835 | 12 | 217 | |
4 | 40MnBc | 850 | ioli | 500 | Amanzi, ioli | 980 | 785 | 10 | 207 | |
5 | 45MnBc | 840 | ioli | 500 | Amanzi, ioli | 1030 | 835 | 9 | 217 | |
6 | 20Mn2bc'f | 880 | ioli | 200 | Amanzi, umoya | 980 | 785 | 10 | 187 | |
7 | 20CrdJ | 880 | 800 | Amanzi, ioli | 200 | Amanzi, umoya | 835 | 540 | 10 | 179 |
785 | 490 | 10 | 179 | |||||||
8 | 30Cr | 860 | ioli | 500 | Amanzi, ioli | 885 | 685 | 11 | 187 | |
9 | 35Kr | 860 | ioli | 500 | Amanzi, ioli | 930 | 735 | 11 | 207 | |
10 | 40Cr | 850 | ioli | 520 | Amanzi, ioli | 980 | 785 | 9 | 207 | |
11 | 45Cr | 840 | ioli | 520 | Amanzi, ioli | 1030 | 835 | 9 | 217 | |
12 | 50Cr | 830 | ioli | 520 | Amanzi, ioli | 1080 | 930 | 9 | 229 | |
13 | 38CrSi | 900 | ioli | 600 | Amanzi, ioli | 980 | 835 | 12 | 255 | |
14 | 20CrModJ | 880 | Amanzi, ioli | 500 | Amanzi, ioli | 885 | 685 | 11 | 197 | |
845 | 635 | 12 | 197 | |||||||
15 | 35CrMo | 850 | ioli | 550 | Amanzi, ioli | 980 | 835 | 12 | 229 | |
16 | 42CrMo | 850 | ioli | 560 | Amanzi, ioli | 1080 | 930 | 12 | 217 | |
17 | 38CrMoAld | 940 | Amanzi, ioli | 640 | Amanzi, ioli | 980 | 835 | 12 | 229 | |
930 | 785 | 14 | 229 | |||||||
18 | 50CrVA | 860 | ioli | 500 | Amanzi, ioli | 1 275 | 1 130 | 10 | 255 | |
19 | 2OCrMn | 850 | ioli | 200 | Amanzi, umoya | 930 | 735 | 10 | 187 | |
20 | 20CrMnSif | 880 | ioli | 480 | Amanzi, ioli | 785 | 635 | 12 | 207 | |
21 | 3OCrMnSif | 880 | ioli | 520 | Amanzi, ioli | 1080 | 885 | 8 | 229 | |
980 | 835 | 10 | 229 | |||||||
22 | 35CrMnSiA£ | 880 | ioli | 230 | Amanzi, umoya | 1 620 | 9 | 229 | ||
23 | 20CrMnTie-f | 880 | 870 | ioli | 200 | Amanzi, umoya | 1080 | 835 | 10 | 217 |
24 | 30CrMnTie*f | 880 | 850 | ioli | 200 | Amanzi, umoya | 1 470 | 9 | 229 | |
25 | 12CrNi2 | 860 | 780 | Amanzi, ioli | 200 | Amanzi, umoya | 785 | 590 | 12 | 207 |
26 | 12CrNi3 | 860 | 780 | ioli | 200 | Amanzi, umoya | 930 | 685 | 11 | 217 |
27 | 12Cr2Ni4 | 860 | 780 | ioli | 200 | Amanzi, umoya | 1080 | 835 | 10 | 269 |
28 | 40CrNiMoA | 850 | —- | ioli | 600 | Amanzi, umoya | 980 | 835 | 12 | 269 |
29 | 45CrNiMoVA | 860 | - | ioli | 460 | ioli | 1 470 | 1 325 | 7 | 269 |
a. Ulungelelwaniso oluvumelekileyo uluhlu lobushushu bonyango oludweliswe kwitheyibhile: ukucima ± 15 ℃, ubushushu obuphantsi bobushushu ± 20 ℃, ubushushu obuphezulu bomhlaba obushushu buyi-50 ℃.b. Kuvavanyo lwe-tensile, iisampulu ezinqamlezayo okanye ezinde zinokuthathwa. Kwimeko yokungavumelani, isampuli yelongitudinal isetyenziswa njengesiseko solamlo.c. Insimbi ene-Boron inokuba yinto eqhelekileyo ngaphambi kokucima, kwaye ukushisa okuqhelekileyo akufanele kube phezulu kunokushisa kwayo.d. Ukuhanjiswa ngokweseti yedatha echazwe ngumfaki-sicelo. Xa umceli engakhange achaze, ukuhanjiswa kungenziwa ngokuhambelana nayiphi na idatha. e. Ukucima kokuqala kwentsimbi ye-titanium kunye ne-Ming Meng kunokutshintshwa ngokuqhelekileyo. f. Ukucima i-Isothermal kwi-280 C ~320 C. g. Kuvavanyo lwe-tensile, ukuba i-Rel ayinakulinganiswa, i-Rp0.2 inokulinganiswa endaweni ye-Rel. |
Imfuneko yoVavanyo
Ukwenziwa kweekhemikhali:
Ukolula, Ubulukhuni, Umothuko, Umngqusho, Ukugoba, uvavanyo lwe-Ultrasonic, iEddy yangoku, ukubhaqwa, ukubhaqwa okuvuzayo, iGalvanized