Superheated steam pipe, malaki at maliit na smoke pipe at arch brick pipe,GB9948-2006
Pamantayan:GB9948-2006 | Paggamot sa init: Pagsusupil/pag-normalize/Pagpapainit |
Pangkat ng Baitang: 10, 12CrMo, 15CrMo, 07Crl9Nil0, atbp | Panlabas na Diameter(Bilog): 10 - 1000 Mm |
Kapal: 1 - 100 mm | Application: heat exchange tubes |
Panlabas na Diameter(Bilog): 10 - 1000 mm | Surface Treatment: Bilang Kinakailangan ng Customer |
Haba: Nakapirming haba o random na haba | Pamamaraan: Hot Rolled |
Hugis ng Seksyon: Bilog | Espesyal na Tubo: Makapal na Tubong Pader |
Lugar ng Pinagmulan: China | Paggamit: heat exchange tubes |
Sertipikasyon: ISO9001:2008 | Pagsubok: UT/MT |
Ang mga seamless steel tubes para sa petroleum cracking ay naaangkop sa seamless steel tubes para sa furnace tubes, heat exchange tubes at pressure pipe sa petrochemical industry.
Ang mataas na kalidad ng carbon structural steel grades ay 20g, 20mng at 25mng.
Alloy structural steel grades: 15mog, 20mog, 12crmog
15CrMoG,12Cr2MoG,12CrMoVG, atbp
Grado ng mataas na kalidad na carbon structural steel: 10#、20#
Mataas na kalidad ng carbon structural steel grades : 20g, 20mng at 25mng
Alloy structural steel grades: 15mog, 20mog, 12crmog, 15CrMoG, 12Cr2MoG, atbp
No | Grade | Chemical Component % | |||||||||||
C | Si | Mn | Cr | Mo | Ni | Nb | Ti | V | Cu | P | S | ||
≤ | |||||||||||||
Mataas na Kalidad ng Carbon Structural Steel | 10 | 0. 07-0.13 | 0.17 -0. 37 | 0.35 -0.65 | <0.15 | <0.15 | <0. 25 | — | — | <0. 08 | <0. 20 | 0. 025 | 0. 015 |
20 | 0.17-0. 23 | 0.17 -0. 37 | 0.35 -0.65 | <0. 25 | <0.15 | <0. 25 | — | — | <0. 08 | <0. 20 | 0. 025 | 0. 015 | |
Alloy Structural Steel | 12CrMo | 0. 08-0.15 | 0.17 -0.37 | 0. 40-0. 70 | 0. 40-0. 70 | 0. 40 -0.55 | <0. 30 | — | — | 一 | <0. 20 | 0. 025 | 0. 015 |
15CrMo | 0.12 -0.18 | 0.17-0. 37 | 0.40 -0. 70 | 0. 80-1.1 | 0. 40-0.55 | <0. 30 | — | — | 一 | <0. 20 | 0. 025 | 0. 015 | |
12CrlMo | 0. 08 -0.15 | 0.50 -1. 00 | 0. 30-0.6 | 1.00-1. 50 | 0.45 -0.65 | <0. 30 | — | — | — | <0, 20 | 0. 025 | 0. 015 | |
12CrlMoV | 0. 08-0.15 | 0.17-0. 37 | 0. 40-0. 70 | 0.90-1.2 | 0. 25 -0.35 | <0. 30 | — | — | 0.15 -0. 30 | <0. 20 | 0.025 | 0. 010 | |
12Cr2Mo | 0.08-0.15 | <0. 50 | 0. 40-0. 60 | 2. 00-2. 50 | 0. 90-1.13 | <0. 30 | — | — | 一 | <0. 20 | 0. 025 | 0. 015 | |
12Cr5MoI | <0.15 | <0. 50 | 0.30-0.6 | 4. 00-6 | 0. 45 -0. 60 | <0. 60 | — | — | <0. 20 | 0. 025 | 0. 015 | ||
12Cr5MoNT | |||||||||||||
12Cr9MoI | <0.15 | 0. 25-1. 00 | 0. 30-0. 60 | 8.00 -10. 00 | 0. 90-1.1 | <0. 60 | — | — | — | <0. 20 | 0. 025 | 0, 015 | |
12Cr9MoNT | |||||||||||||
Hindi kinakalawang na init na bakal | 07Crl9Nil0 | 0. 04-0.1 | <1. 00 | <2. 00 | 18. 00-20. 00 | — | 8. 00-11 | — | — | — | — | 0. 030 | 0. 015 |
07Crl8NillNb | 0. 04-0.1 | <1. 00 | <2. 00 | 17. 00-19. 00 | — | 9.00-12. 00 | 8C-1.1 | — | — | — | 0. 030 | 0. 015 | |
07Crl9NillTi | 0. 04-0.1 | <0. 75 | <2. 00 | 17.00-20. 00 | — | 9. 00~13. 00 | — | 4C-0. 60 | 一 | 一 | 0.03 | 0. 015 | |
022Crl7Nil2Mo2 | <0. 030 | <1. 00 | <2. 00 | 16. 00-18. 00 | 2. 00-3. 00 | 10. 00 -14. 00 | — | 一 | 一 | — | 0.03 | 0. 015 |
Hindi | makunat MPa | Magbigay MPa | Mahaba pagkatapos ng bali A/% | Enerhiya ng pagsipsip ng shork kv2/j | Numero ng katigasan ng Brinell | ||
portrait | transver | portrait | transver | ||||
hindi bababa sa | hindi hihigit sa | ||||||
10 | 335〜475 | 205 | 25 | 23 | 40 | 27 | |
20 | 410〜550 | 245 | 24 | 22 | 40 | 27 | |
12CrMo | 410〜560 | 205 | 21 | 19 | 40 | 27 | 156 HBW |
15CrMo | 440〜640 | 295 | 21 | 19 | 40 | 27 | 170 HBW |
12CrlMo | 415〜560 | 205 | 22 | 20 | 40 | 27 | 163 HBW |
12CrlMoV | 470〜640 | 255 | 21 | 19 | 40 | 27 | 179 HBW |
12Cr2Mo | 450~600 | 280 | 22 | 20 | 40 | 27 | 163 HBW |
12Cr5MoI | 415〜590 | 205 | 22 | 20 | 40 | 27 | 163 HBW |
12Cr5MoNT | 480〜640 | 280 | 20 | 18 | 40 | 27 | — |
12Cr9MoI | 460〜640 | 210 | 20 | 18 | 40 | 27 | 179 HBW |
12Cr9MoNT | 590—740 | 390 | 18 | 16 | 40 | 27 | |
O7Crl9NilO | 2520 | 205 | 35 | 187 HBW | |||
07Crl8NillNb | >520 | 205 | 35 | — | 187 HBW | ||
07Crl9NillTi | >520 | 205 | 35 | — | — | 187 HBW | |
022Crl7Nil2Mo2 | >485 | 170 | 35 | 一 | — | 187 HBW | |
Para sa bakal na may kapal ng pader na mas mababa sa 5mm tube, huwag gumawa ng hardness experiment |
Pagsusuri ng haydroliko
Ang haydroliko na pagsubok ay isasagawa para sa mga bakal na tubo nang paisa-isa. Ang pinakamataas na presyon ng pagsubok ay 20 MPa. Sa ilalim ng presyon ng pagsubok, ang oras ng pagpapapanatag ay hindi dapat mas mababa sa 10 s, at hindi pinapayagan ang pagtagas ng bakal na tubo.
Pagsusulit sa pagyupi
Ang flattening test ay dapat isagawa para sa steel pipe na may panlabas na diameter na higit sa 22 mm
Pagsubok sa paglalagablab
Ang mataas na kalidad na carbon structural steel at hindi kinakalawang (heat-resistant) steel pipe na may panlabas na diameter na hindi hihigit sa 76 mm at ang kapal ng pader na hindi hihigit sa 8 mm ay sasailalim sa pagpapalawak ng pagsubok. Ang flaring test ay dapat isagawa sa temperatura ng silid. Ang panlabas na diameter ng flaring rate ng sample pagkatapos ng tuktok na core taper ay 60% ng flaring ay dapat matugunan ang mga kinakailangan ng talahanayan 7. Walang mga bitak o bitak ang pinapayagan sa sample pagkatapos ng flaring. Ayon sa mga kinakailangan ng demander at nabanggit sa kontrata, ang haluang metal na istruktura na bakal ay maaari ding gamitin para sa pagpapalawak ng pagsubok.
Hindi mapanirang pagsubok
Ang mga bakal na tubo ay sasailalim sa ultrasonic flaw detection nang paisa-isa alinsunod sa mga probisyon ng GB / T 5777-2008. Ayon sa mga kinakailangan ng demander, ang iba pang mga hindi mapanirang pagsubok ay maaaring idagdag pagkatapos ng negosasyon sa pagitan ng supplier at ng demander at ipinahiwatig sa kontrata.
Intergranular corrosion test
Ang intergranular corrosion test ay dapat isagawa para sa stainless (heat-resistant) steel pipe. Ang paraan ng pagsubok ay dapat alinsunod sa mga probisyon ng Chinese method E sa GB / T 4334-2008, at hindi pinapayagan ang intergranular corrosion tendency pagkatapos ng pagsubok.
Pagkatapos ng negosasyon sa pagitan ng supplier at ng demander, at nabanggit sa kontrata, ang demander ay maaaring magtalaga ng iba pang mga pamamaraan ng pagsubok sa kaagnasan.
Langis, petrochemical, high pressure boiler, espesyal na paggamit ng seamless tube boiler seamless tube, geological seamless steel tube at oil seamless tube.
Chemical Component
tatak | Chemical Component(%) | ||||||||
C | Mn | Si | Cr | Mo | Ni | Nb+Ta | S | P | |
15CrMo | 0.12~0.18 | 0.40~0.70 | 0.17~0.37 | 0.80~1.10 | 0.40~0.55 | ≤0.30 | _ | ≤0.035 | ≤0.035 |
Mechanical Property
tatak | makunat MPa | Magbigay MPa | Pagpahaba(%) |
15CrMo | 440~640 | 295 | 22 |